<?xml version="1.0" encoding="UTF-8"?>
<!DOCTYPE article PUBLIC "-//TaxonX//DTD Taxonomic Treatment Publishing DTD v0 20100105//EN" "../../nlm/tax-treatment-NS0.dtd">
<article xmlns:mml="http://www.w3.org/1998/Math/MathML" xmlns:xlink="http://www.w3.org/1999/xlink" xmlns:xsi="http://www.w3.org/2001/XMLSchema-instance" xmlns:tp="http://www.plazi.org/taxpub" article-type="research-article" dtd-version="3.0" xml:lang="en">
  <front>
    <journal-meta>
      <journal-id journal-id-type="publisher-id">80</journal-id>
      <journal-id journal-id-type="index">urn:lsid:arphahub.com:pub:3CDB4662-2EEC-55B0-878A-88F876A7F403</journal-id>
      <journal-title-group>
        <journal-title xml:lang="en">Modern Electronic Materials</journal-title>
        <abbrev-journal-title xml:lang="en">MoEM</abbrev-journal-title>
      </journal-title-group>
      <issn pub-type="ppub">2452-2449</issn>
      <issn pub-type="epub">2452-1779</issn>
      <publisher>
        <publisher-name>NUST MISiS</publisher-name>
      </publisher>
    </journal-meta>
    <article-meta>
      <article-id pub-id-type="doi">10.3897/j.moem.6.2.54295</article-id>
      <article-id pub-id-type="publisher-id">54295</article-id>
      <article-categories>
        <subj-group subj-group-type="heading">
          <subject>Research Article</subject>
        </subj-group>
      </article-categories>
      <title-group>
        <article-title>Enhancement of piezoelectric properties of lithium niobate thin films by different annealing parameters</article-title>
      </title-group>
      <contrib-group>
        <contrib contrib-type="author" xlink:type="simple" corresp="no">
          <name name-style="western">
            <surname>Zhukov</surname>
            <given-names>Roman N.</given-names>
          </name>
          <xref ref-type="aff" rid="A1">1</xref>
        </contrib>
        <contrib contrib-type="author" xlink:type="simple" corresp="no">
          <name name-style="western">
            <surname>Kushnerev</surname>
            <given-names>K.S.</given-names>
          </name>
          <xref ref-type="aff" rid="A1">1</xref>
        </contrib>
        <contrib contrib-type="author" xlink:type="simple" corresp="no">
          <name name-style="western">
            <surname>Kiselev</surname>
            <given-names>Dmitry A.</given-names>
          </name>
          <xref ref-type="aff" rid="A1">1</xref>
          <uri content-type="orcid">https://orcid.org/0000-0003-1047-3007</uri>
        </contrib>
        <contrib contrib-type="author" xlink:type="simple" corresp="no">
          <name name-style="western">
            <surname>Ilina</surname>
            <given-names>Tatiana S.</given-names>
          </name>
          <xref ref-type="aff" rid="A1">1</xref>
        </contrib>
        <contrib contrib-type="author" xlink:type="simple" corresp="no">
          <name name-style="western">
            <surname>Kubasov</surname>
            <given-names>Ilya V.</given-names>
          </name>
          <xref ref-type="aff" rid="A1">1</xref>
          <uri content-type="orcid">https://orcid.org/0000-0002-6569-466X</uri>
        </contrib>
        <contrib contrib-type="author" xlink:type="simple" corresp="no">
          <name name-style="western">
            <surname>Kislyuk1</surname>
            <given-names>Alexander M.</given-names>
          </name>
          <xref ref-type="aff" rid="A1">1</xref>
        </contrib>
        <contrib contrib-type="author" xlink:type="simple" corresp="yes">
          <name name-style="western">
            <surname>Malinkovich</surname>
            <given-names>Mikhail D.</given-names>
          </name>
          <xref ref-type="aff" rid="A1">1</xref>
          <email xlink:type="simple">malinkovich@yandex.ru</email>
        </contrib>
        <contrib contrib-type="author" xlink:type="simple" corresp="no">
          <name name-style="western">
            <surname>Parkhomenko</surname>
            <given-names>Yuri N.</given-names>
          </name>
          <xref ref-type="aff" rid="A1">1</xref>
        </contrib>
      </contrib-group>
      <aff id="A1">
        <label>1</label>
        <addr-line content-type="verbatim">National University of Science and Technology MISiS, 4 Leninsky Prospekt, Moscow 119049, Russia</addr-line>
        <institution>National University of Science and Technology MISiS</institution>
        <addr-line content-type="city">Moscow</addr-line>
        <country>Russia</country>
      </aff>
      <author-notes>
        <fn fn-type="corresp">
          <p>Corresponding author: Mikhail D. Malinkovich (malinkovich@yandex.ru)</p>
        </fn>
      </author-notes>
      <pub-date pub-type="collection">
        <year>2020</year>
      </pub-date>
      <pub-date pub-type="epub">
        <day>30</day>
        <month>06</month>
        <year>2020</year>
      </pub-date>
      <volume>6</volume>
      <issue>2</issue>
      <fpage>47</fpage>
      <lpage>52</lpage>
      <uri content-type="arpha" xlink:href="http://openbiodiv.net/126BEC7F-EEE5-589C-B16E-32140C54CABD">126BEC7F-EEE5-589C-B16E-32140C54CABD</uri>
      <history>
        <date date-type="received">
          <day>14</day>
          <month>05</month>
          <year>2020</year>
        </date>
        <date date-type="accepted">
          <day>25</day>
          <month>06</month>
          <year>2020</year>
        </date>
      </history>
      <permissions>
        <copyright-statement>Roman N. Zhukov, K.S. Kushnerev, Dmitry A. Kiselev, Tatiana S. Ilina, Ilya V. Kubasov, Alexander M. Kislyuk, Mikhail D. Malinkovich, Yuri N. Parkhomenko</copyright-statement>
        <license license-type="creative-commons-attribution" xlink:href="http://creativecommons.org/licenses/by/4.0/" xlink:type="simple">
          <license-p>This is an open access article distributed under the terms of the Creative Commons Attribution License (CC BY 4.0), which permits unrestricted use, distribution, and reproduction in any medium, provided the original author and source are credited.</license-p>
        </license>
      </permissions>
      <abstract>
        <label>Abstract</label>
        <p>Piezoelectric materials with useful properties find a wide range of applications including opto- and acousto- electronics. Lithium niobate in the form of a thin film is one of those promising materials and has a potential to improve ferroelectric random access memories devices, optical waveguides or acoustic delay lines by virtue of its physical characteristics, e.g. electro-optic coefficient, acoustic velocity, refractive indices etc. The key challenge to overcome is lithium nonstoichiometry as it leads to the appearance of parasite phases and thus aggravates physical and structural properties of a film. According to literature data, in order to obtain microcrystalline piezoelectric phase in previously amorphous films a set of methods is used. In our case we tried to synthesize LN films using congruent target and non-heated silicon substrate and then attain the piezoelectric phase by different annealing parameters. Afterwards LN films were compared to the ones synthesized on the silicon substrate with an additional buffer layer of platinum. Samples were studied by scanning probe microscope. Self-polarization vectors were defined. Based on domain structure images, the histograms of distribution of piezoresponse signals were built.</p>
      </abstract>
      <kwd-group>
        <label>Keywords</label>
        <kwd>Lithium niobate</kwd>
        <kwd>rf magnetron sputtering</kwd>
        <kwd>post-growth heat treatment</kwd>
        <kwd>scanning probe microscopy</kwd>
        <kwd>piezoelectric force microscopy</kwd>
        <kwd>histogram of distribution of vertical and lateral piezoresponse</kwd>
      </kwd-group>
    </article-meta>
  </front>
  <body>
    <sec sec-type="1. Introduction" id="SECID0EBF">
      <title>1. Introduction</title>
      <p>Piezoelectrics are promising materials for various applications in actual and potential electronics, in particular opto- and acousto- electronics and guided photonics. One of the most substantial and interesting piezoelectric materials is lithium niobate (LiNbO<sub>3</sub>) [<xref ref-type="bibr" rid="B1">1</xref>, <xref ref-type="bibr" rid="B2">2</xref>]. This compound comprises unique and exceptional properties eligible to be implemented into diverse devices. Along with thermally stable piezoelectric modules and pyroelectric coefficients [<xref ref-type="bibr" rid="B1">1</xref>] this material also possesses unique optical properties, which have a potential to upgrade optical waveguides, ferroelectric random access memories, high dielectric constant capacitors, acoustic delay lines, microwave tunable devices. Among those properties are electromechanical coupling coefficient (K<sup>2</sup>) [<xref ref-type="bibr" rid="B3">3</xref>], electro-optic coefficient, acoustic velocity and refractive indices; thus, it is widely used in many diverse devices such as next-generation of high-frequency and/or wide-band RF filters or tuneable frequency filters adapted to the fifth generation of networks [<xref ref-type="bibr" rid="B4">4</xref>]. However physical and structural properties of LN are highly dependent on the lithium nonstoichiometry [<xref ref-type="bibr" rid="B5">5</xref>, <xref ref-type="bibr" rid="B6">6</xref>]. For instance, deficiency of lithium <!--PageBreak-->atoms substantially affects Curie temperature [<xref ref-type="bibr" rid="B7">7</xref>], elastic constants [<xref ref-type="bibr" rid="B8">8</xref>], density [<xref ref-type="bibr" rid="B9">9</xref>, <xref ref-type="bibr" rid="B10">10</xref>], refractive indices [<xref ref-type="bibr" rid="B11">11</xref>], birefringence and many other characteristics. Therefore, the composition of the films has to be precisely controlled for large-scale devices production. Lithium is a light element and (after the growth of the film) lack of its atoms in LN compound leads to emergence of parasite non-piezoelectric phases (such as LiNb<sub>3</sub>O<sub>8</sub>) [<xref ref-type="bibr" rid="B12">12</xref>]. A number of steps were made to prevent this process, such as, heating the substrate or using of stoichiometric target or even target with lithium excess. Another way to improve the quality of the film is to use a substrate with metal buffer layers. In our case we used congruent target and tried to obtain films on a non-heated silicon substrate to minimize lithium volatility and then enhance film’s piezoelectric properties and crystallinity by post-growth heat treatment. Therefore, the goal of this work was to find optimal annealing parameters of an initially amorphous LN thin film (grown on a silicon substrate without any additional buffer layers) in order to obtain microcrystalline piezoelectric phase.</p>
    </sec>
    <sec sec-type="2. Experimental" id="SECID0EFH">
      <title>2. Experimental</title>
      <p>For the experimental research the thin film of LN was grown by RF magnetron sputtering. The deposition of the thin film was performed on a silicon substrate of (111) orientation in atmosphere of argon and oxygen with ratio of 1:1. The substrate was preliminarily cleaned with argon gun for 5 minutes before the beginning of deposition process.</p>
      <p>All samples were produced by magnetron sputtering in SUNPLA 40TM vacuum chamber (South Korea) [<xref ref-type="bibr" rid="B13">13</xref>]. The magnetron power equaled 150W with the pressure in vacuum chamber where deposition process was carried out being 0.5 Pa. The film thickness equaled 300 nm. Once the growth process was accomplished, initially amorphous films were annealed in order to improve the crystallinity as well as to increase the share of piezoelectric phase of (R3c) LiNbO<sub>3</sub> in the film. Post-growth heat treatment parameters were different for each sample.</p>
      <p>The annealing was performed in the muffle furnace at the temperature of 700 °C, the optimal annealing temperature: it lowers thin film’s surface roughness and contributes to the highest degree to the structuring of the ferroelectric phase [<xref ref-type="bibr" rid="B13">13</xref>]. Samples 1 and 2 were both heated to 700 °C for 12 minutes, afterwards Sample 1 was held at this temperature for 1 more minute while Sample 2 – for 5 minutes.</p>
      <p>Samples 3 and 4 were heated to 700 °C quicker – for 5 minutes. Once the process was completed Sample 3 was removed from the furnace and Sample 4 was held at that temperature for one more minute before it was taken out from the furnace.</p>
      <p>Samples 5 and 6 were heated to 700 °C for 2 minutes. In this case Sample 5 was right afterwards removed from the furnace while Sample 6 was held there for 1 minute at the same temperature of 700 °C.</p>
      <p>All six samples were cooled naturally in the atmosphere.</p>
      <p>Studies of topography, domain structure and residual hysteresis loops were carried out on SEM with the help of MFP-3D SA scanning probe microscope (Аsylum Research, USA) using Asyelec-02 cantilever (Asylum Research, USA). The subsequent analysis of topography images with WxSM and Gwyddion programs allowed to determine roughness and grain size of the examined thin films. Visualization of domain structure was realized by piezoelectric force microscopy.</p>
      <p>Domain structure images were obtained by applying AC voltage of 5V, frequency of 142 kHz by phase shift of 270⁰ to cantilever.</p>
      <p>With the help of scanning probe microscopy, it is possible to define the direction of self-polarization P<sub>s</sub> in examined materials. For this purpose, the histograms of the distribution of piezoresponse signals based on domain structure images were built.</p>
    </sec>
    <sec sec-type="3. Results and discussion" id="SECID0ECAAC">
      <title>3. Results and discussion</title>
      <p>In order to determine the direction of polarization P<sub>s</sub>, once a piezoresponse magnitude image is obtained, a histogram was generated and the peak values were noted. Moreover, the distribution of piezoresponse signals allows to make a conclusion on the volume of piezoelectric phase in thin films samples.</p>
      <p>First pair of samples (1 and 2) was slowly heated up to 700 °C for 12 minutes with holding time of 1 and 5 minutes respectively. The temperature of 700 °C was chosen with regards to the work of D. A. Kiselev, R. N. Zhukov et al [<xref ref-type="bibr" rid="B13">13</xref>], where a considerable share of non-piezoelectric LiNb<sub>3</sub>O<sub>8</sub> phase was detected at higher (1000 °C) temperature while annealing at lower temperature (550 °C) led to decrease in film crystallinity. The corresponding diffractogram is presented at Figure <xref ref-type="fig" rid="F3">3</xref>. As the histograms show (Figure <xref ref-type="fig" rid="F1">1a, b</xref>) there are several not intensive peaks different from zero. They indicate a small part of domains with multidirectional self-polarization vectors. Nevertheless, the intensity of zero-peak demonstrates the presence of a non-piezoelectric phase of high volume in LN films. The intensity of piezoresponse of both samples in lateral and vertical direction was almost the same with a maximum of 5,0E8 arbitrary units.</p>
      <p>In order to decrease the effect of lithium volatility during the annealing process it was suggested to reduce both heating and holding times for Samples 3 and 4. As the histograms show (Figure <xref ref-type="fig" rid="F1">1c, d</xref>), both samples’ zero peaks in vertical direction moved slightly away from zero, while these peaks were not as narrow as for Samples 1 and 2. This is a good sign of possible presence of piezoelectric phase. However, self-polarization vector forwarded from the interface has an extremely low value.</p>
      <p>Samples 5 and 6 were heated to 700 °C even quicker (in 2 minutes) but their histograms (Figure <xref ref-type="fig" rid="F2">2 e, f</xref>) reveal an almost complete absence of piezoelectric phase in LN films.</p>
      <p>Possibly the films could not crystallize for such a short time and a part of the samples was still amorphous or far enough from microcrystalline structure.</p>
      <fig id="F1" position="float" orientation="portrait">
        <object-id content-type="arpha">F3DC1F22-F972-5221-B6CE-CBE62F116328</object-id>
        <label>Figure 1.</label>
        <caption>
          <p>Histograms of distribution of piezoresponse signals for Samples 1–4 (a,b, c, d respectively). Blue line is the vertical piezoresponse, red line is the lateral piezoresponse.</p>
        </caption>
        <graphic xlink:href="moem-06-e54295-g001.jpg" position="float" orientation="portrait" xlink:type="simple" id="oo_452713.jpg">
          <uri content-type="original_file">https://binary.pensoft.net/fig/452713</uri>
        </graphic>
      </fig>
      <fig id="F2" position="float" orientation="portrait">
        <object-id content-type="arpha">25CAC652-6912-554C-9293-0D124D3FAC11</object-id>
        <label>Figure 2.</label>
        <caption>
          <p>Histograms of distribution of piezoresponse signals for Samples 5–6 (e,f respectively). Blue line is the vertical piezoresponse, red line is the lateral piezoresponse.</p>
        </caption>
        <graphic xlink:href="moem-06-e54295-g002.jpg" position="float" orientation="portrait" xlink:type="simple" id="oo_452714.jpg">
          <uri content-type="original_file">https://binary.pensoft.net/fig/452714</uri>
        </graphic>
      </fig>
      <fig id="F3" position="float" orientation="portrait">
        <object-id content-type="arpha">BCC842E8-1AE0-5D19-9B98-C744FE349C36</object-id>
        <label>Figure 3.</label>
        <caption>
          <p>X-ray diffraction patterns of an as-grown LiNbO<sub>3</sub> film and films heat-treated at different temperatures from the work of Kiselev et al. [13].</p>
        </caption>
        <graphic xlink:href="moem-06-e54295-g003.jpg" position="float" orientation="portrait" xlink:type="simple" id="oo_452715.jpg">
          <uri content-type="original_file">https://binary.pensoft.net/fig/452715</uri>
        </graphic>
      </fig>
      <!--PageBreak-->
      <!--PageBreak-->
      <p>The roughness of all samples varied between 1.4–2.4 nm. Figure <xref ref-type="fig" rid="F4">4</xref> displays the topography and domain structures of Samples 1–4, while Figure <xref ref-type="fig" rid="F5">5</xref> shows the same for Samples 5 and 6.</p>
      <p>The combined results of heating and holding times, roughness and intensity can be observed from the Table <xref ref-type="table" rid="T1">1</xref>.</p>
      <p>According to all the histograms presented earlier in the paper (Figures <xref ref-type="fig" rid="F1">1</xref> and <xref ref-type="fig" rid="F2">2</xref>), we can conclude that it is extremely challenging to obtain successful lithium niobate films with satisfying piezoelectric characteristics on “clean” silicon substrates. The probable reason for this is that there is always a layer of silicon oxide SiO<sub>x</sub> on the surface of silicon unless it is purposely removed before lithium niobate is deposited. Silicon oxide is an effective getter for Li<sub>2</sub>O [<xref ref-type="bibr" rid="B14">14</xref>], which promotes lithium niobate film <!--PageBreak-->depletion by lithium. Thus, it can be expected that more stoichiometric compound of a lithium niobate film on the surface of silicon can be obtained by generating an anti-diffusion barrier between lithium niobate and the substrate. For example, a thin layer of platinum can be used as an anti-diffusion barrier preventing the loss of lithium from the film [<xref ref-type="bibr" rid="B15">15</xref>]. Figure <xref ref-type="fig" rid="F6">6</xref> shows the distribution histogram of piezoresponse signal received on a lithium niobate film containing a platinum sublayer [<xref ref-type="bibr" rid="B16">16</xref>], compared with the result obtained on a film without a platinum sublayer. It can be observed that piezoresponse and, therefore, the part of the piezoelectric phase on films with a platinum sublayer is much larger while the nonpiezoelectric phase is practically absent which indicates sufficiently high quality of such material.</p>
      <fig id="F4" position="float" orientation="portrait">
        <object-id content-type="arpha">CC36D9E4-FD23-5FDB-9C2B-2FCD696E26D3</object-id>
        <label>Figure 4.</label>
        <caption>
          <p>Topography and domain structures of samples 1–4 (a, b, c, d). From left to right: topography, VPFM, LPFM.</p>
        </caption>
        <graphic xlink:href="moem-06-e54295-g004.jpg" position="float" orientation="portrait" xlink:type="simple" id="oo_452716.jpg">
          <uri content-type="original_file">https://binary.pensoft.net/fig/452716</uri>
        </graphic>
      </fig>
      <fig id="F5" position="float" orientation="portrait">
        <object-id content-type="arpha">D02A1389-509E-56FC-9AEE-A2755ECEFC39</object-id>
        <label>Figure 5.</label>
        <caption>
          <p>Topography and domain structures of Samples 5 and 6 (e and f). From left to right: topography, VPFM, LPFM.</p>
        </caption>
        <graphic xlink:href="moem-06-e54295-g005.jpg" position="float" orientation="portrait" xlink:type="simple" id="oo_452717.jpg">
          <uri content-type="original_file">https://binary.pensoft.net/fig/452717</uri>
        </graphic>
      </fig>
      <table-wrap id="T1" position="float" orientation="portrait">
        <label>Table 1.</label>
        <caption>
          <p>The combined results of annealing parameters and following roughness and intensity examination.</p>
        </caption>
        <table id="TID0EAAAE" rules="all">
          <tbody>
            <tr>
              <th rowspan="1" colspan="1">Sample</th>
              <th rowspan="1" colspan="1">Heating time, minutes (up to 700 °C)</th>
              <th rowspan="1" colspan="1">Holding time, minutes (at 700 °C)</th>
              <th rowspan="1" colspan="1">Roughness, nm</th>
              <th rowspan="1" colspan="1">Intensity, arb. units</th>
            </tr>
            <tr>
              <td rowspan="1" colspan="1">1 (a)</td>
              <td rowspan="1" colspan="1">12</td>
              <td rowspan="1" colspan="1">1</td>
              <td rowspan="1" colspan="1">1.88</td>
              <td rowspan="1" colspan="1">5.0E8</td>
            </tr>
            <tr>
              <td rowspan="1" colspan="1">2 (b)</td>
              <td rowspan="1" colspan="1">12</td>
              <td rowspan="1" colspan="1">5</td>
              <td rowspan="1" colspan="1">2.35</td>
              <td rowspan="1" colspan="1">5.2E8</td>
            </tr>
            <tr>
              <td rowspan="1" colspan="1">3 (c)</td>
              <td rowspan="1" colspan="1">5</td>
              <td rowspan="1" colspan="1">0</td>
              <td rowspan="1" colspan="1">1.42</td>
              <td rowspan="1" colspan="1">5.5E8</td>
            </tr>
            <tr>
              <td rowspan="1" colspan="1">4 (d)</td>
              <td rowspan="1" colspan="1">5</td>
              <td rowspan="1" colspan="1">1</td>
              <td rowspan="1" colspan="1">1.54</td>
              <td rowspan="1" colspan="1">6.0E8</td>
            </tr>
            <tr>
              <td rowspan="1" colspan="1">5 (e)</td>
              <td rowspan="1" colspan="1">2</td>
              <td rowspan="1" colspan="1">0</td>
              <td rowspan="1" colspan="1">2.00</td>
              <td rowspan="1" colspan="1">7.8E8</td>
            </tr>
            <tr>
              <td rowspan="1" colspan="1">6 (f)</td>
              <td rowspan="1" colspan="1">2</td>
              <td rowspan="1" colspan="1">1</td>
              <td rowspan="1" colspan="1">2.22</td>
              <td rowspan="1" colspan="1">1.0E9</td>
            </tr>
          </tbody>
        </table>
      </table-wrap>
      <fig id="F6" position="float" orientation="portrait">
        <object-id content-type="arpha">4B83CAE1-C89E-52E9-AE79-68B21B9BC3E8</object-id>
        <label>Figure 6.</label>
        <caption>
          <p>Histograms of distribution of piezoresponse signals for LiNbO<sub>3</sub>/SiO<sub>x</sub>/Si (line 1) and LiNbO<sub>3</sub>/Pt/Si (line 2) heterostructures [14].</p>
        </caption>
        <graphic xlink:href="moem-06-e54295-g006.jpg" position="float" orientation="portrait" xlink:type="simple" id="oo_452718.jpg">
          <uri content-type="original_file">https://binary.pensoft.net/fig/452718</uri>
        </graphic>
      </fig>
    </sec>
    <sec sec-type="4. Conclusion" id="SECID0E2CAC">
      <title>4. Conclusion</title>
      <p>By changing annealing parameters (heating and holding times) we tried to enhance piezoelectric properties of lithium niobate thin films grown on a “cold” Si (111) substrate by RF magnetron sputtering. According to piezoresponse signal distribution there is a small volume of differently oriented domains (which embody the existence of piezoelectric phase) in samples heated up to 700 °C for 12 minutes (with holding times of 1 and 5 minutes) and in samples heated for 5 minutes (with holding times of 0 and 1 minute). The roughness of those films is extremely low and lies between 1.4 and 2.4 nm.</p>
      <p>Nevertheless, generally we can reveal that samples contain an extremely small amount of piezoelectric component which might be the consequence of poorly selected annealing parameters. Presumably at shortening heating time LN film is unable to form a stable multi-domain structure and <!--PageBreak-->predominant formation of isolated single grains happens. Though it would be tremendously beneficial and advantageous to obtain lithium niobate films on silicon substrates without any additional layers, the task seems immensely challenging. We conducted a series of annealing experiments and came to the conclusion that the most successful LN films were grown on the substrates with such buffer layers as platinum. Those films contained a larger amount of piezoelectric phase and showed better piezoresponse.</p>
      <p>Further experiments on the selection of optimal annealing parameters are necessary for enhancement and increase of the piezoelectric phase in lithium niobate thin films.</p>
    </sec>
  </body>
  <back>
    <ack>
      <title>Acknowledgements</title>
      <p>The work was supported by the Ministry of Science and Higher Education of the Russian Federation as a part of the State Assignment (basic research, Project No. 0718-2020-0031 “New magnetoelectric composite materials based on oxide ferroelectrics having an ordered domain structure: production and properties”). The studies were performed on the equipment of Center for Shared Use “Materials Science and Metallurgy” at the National University of Science and Technology “MISiS”.</p>
    </ack>
    <ref-list>
      <title>References</title>
      <ref id="B1">
        <label>1</label>
        <mixed-citation xlink:type="simple">Kuzminov Y.S. <italic>Electroopticheskiy i nelineynoopticheskiy kristall niobata litiya</italic> [Electrooptical and Nonlinear Optical Lithium Niobate Crystal]. Moscow: Nauka, 1987: 263 p. (In Russ.)</mixed-citation>
      </ref>
      <ref id="B2">
        <label>2</label>
        <mixed-citation xlink:type="simple">Volk T., Wohlecke M. Lithium Niobate: Defects, Photorefraction and Ferroelectric Switching, Springer Science &amp; Business Media, 2008: 250 p.</mixed-citation>
      </ref>
      <ref id="B3">
        <label>3</label>
        <mixed-citation xlink:type="simple">Yamada K., Takemura H., Inoue Y., Omi T., Matsumura S. Effect of Li/Nb Ratio on the SAW Velocity of 128°Y–X LiNbO<sub>3</sub> Wafers. <italic>Japanese Journal of Applied Physics</italic>. 1987; 26-2: 219–222. <ext-link xlink:type="simple" ext-link-type="doi" xlink:href="10.7567/JJAPS.26S2.219">https://doi.org/10.7567/JJAPS.26S2.219</ext-link></mixed-citation>
      </ref>
      <ref id="B4">
        <label>4</label>
        <mixed-citation xlink:type="simple">Bartasyte A., Margueron S., Baron T., Oliveri S., Boulet P. Toward High-Quality Epitaxial LiNbO<sub>3</sub> and LiTaO<sub>3</sub> Thin Films for Acoustic and Optical Applications. <italic>Advanced Materials Interfaces</italic>. 2017; 4 (8): 1600998 (36 pp.). <ext-link xlink:type="simple" ext-link-type="doi" xlink:href="10.1002/admi.201600998">https://doi.org/10.1002/admi.201600998</ext-link></mixed-citation>
      </ref>
      <ref id="B5">
        <label>5</label>
        <mixed-citation xlink:type="simple">Bordui P.F., Norwood R.G., Bird C.D., Calvert G.D. Compositional uniformity in growth and poling of large-diameter lithium niobate crystals. <italic>Journal of Crystal Growth</italic>. 1991; 113(1-2): 61–68. DOI: <ext-link xlink:type="simple" ext-link-type="doi" xlink:href="10.1016/0022-0248(91)90009-T">10.1016/0022-0248(91)90009-T</ext-link></mixed-citation>
      </ref>
      <ref id="B6">
        <label>6</label>
        <mixed-citation xlink:type="simple">Bordui P.F., Norwood R.G., Bird C.D., Carella J.T. Stoichiometry issues in single‐crystal lithium tantalate. <italic>Journal of Applied Physics</italic>. 1995; 78(7): 4647–4650. <ext-link xlink:type="simple" ext-link-type="doi" xlink:href="10.1063/1.359811">https://doi.org/10.1063/1.359811</ext-link></mixed-citation>
      </ref>
      <ref id="B7">
        <label>7</label>
        <mixed-citation xlink:type="simple">Tian L., Gopalan V., Galambos L. Domain reversal in stoichiometric LiTaO<sub>3</sub> prepared by vapor transport equilibration. <italic>Applied Physics Letters</italic>. 2004; 85(19): 4445–4447. <ext-link xlink:type="simple" ext-link-type="doi" xlink:href="10.1063/1.1814436">https://doi.org/10.1063/1.1814436</ext-link></mixed-citation>
      </ref>
      <ref id="B8">
        <label>8</label>
        <mixed-citation xlink:type="simple">Kushibiki J., Takanaga I., Komatsuzaki S., Ujiie T. Chemical composition dependences of the acoustical physical constants of LiNbO<sub>3</sub> and LiTaO<sub>3</sub> single crystals. <italic>Journal of Applied Physics</italic>. 2002; 91(10): 6341–6349. <ext-link xlink:type="simple" ext-link-type="doi" xlink:href="10.1063/1.1467608">https://doi.org/10.1063/1.1467608</ext-link></mixed-citation>
      </ref>
      <ref id="B9">
        <label>9</label>
        <mixed-citation xlink:type="simple">Iyi N., Kitamura K., Izumi F., Yamamoto J.K., Hayashi T., Asano H., Kimura S. Comparative study of defect structures in lithium niobate with different compositions. <italic>Journal of Solid State Chemistry</italic>. 1992; 101(2): 340–352. <ext-link xlink:type="simple" ext-link-type="doi" xlink:href="10.1016/0022-4596(92)90189-3">https://doi.org/10.1016/0022-4596(92)90189-3</ext-link></mixed-citation>
      </ref>
      <ref id="B10">
        <label>10</label>
        <mixed-citation xlink:type="simple">Kushibiki J., Ohashi Y., Hirohashi J. Ultrasonic microspectroscopy of congruent LiNbO<sub>3</sub> crystals. <italic>Journal of Applied Physics</italic>. 2005; 98(12): 123507 (1-8). <ext-link xlink:type="simple" ext-link-type="doi" xlink:href="10.1063/1.2146076">https://doi.org/10.1063/1.2146076</ext-link>.</mixed-citation>
      </ref>
      <ref id="B11">
        <label>11</label>
        <mixed-citation xlink:type="simple">Schlarb U., Betzler K. Refractive indices of lithium niobate as a function of wavelength and composition. <italic>Journal of Applied Physics</italic>. 1993; 73(7): 3472–3476. <ext-link xlink:type="simple" ext-link-type="doi" xlink:href="10.1063/1.352951">https://doi.org/10.1063/1.352951</ext-link></mixed-citation>
      </ref>
      <ref id="B12">
        <label>12</label>
        <mixed-citation xlink:type="simple">Prezas P. R. S, Graça M. P. F Structural Characterization of Lithium Niobate Nanoparticles Prepared by the Sol-Gel Process, Using X-Ray and Raman Spectroscopy and Scanning Electron Microscopy. Applications of Molecular Spectroscopy to Current Research in the Chemical and Biological Sciences, 2016. <ext-link xlink:type="simple" ext-link-type="doi" xlink:href="10.5772/64395">http://dx.doi.org/10.5772/64395</ext-link></mixed-citation>
      </ref>
      <ref id="B13">
        <label>13</label>
        <mixed-citation xlink:type="simple">Kiselev D.A., Zhukov R.N., Bykov A.S., Voronova M.I., Shcherbachev K.D., Malinkovich M.D., Parkhomenko Y.N. Effect of annealing on the structure and phase composition of thin electro-optical lithium niobate films. <italic>Inorganic Materials</italic>, 2014; 50(4): 419–422. <ext-link xlink:type="simple" ext-link-type="doi" xlink:href="10.1134/s0020168514040074">https://doi.org/10.1134/s0020168514040074</ext-link></mixed-citation>
      </ref>
      <ref id="B14">
        <label>14</label>
        <mixed-citation xlink:type="simple">Yamamoto K., Mizuuchi K., Takeshige K., Sasai Y., Taniuchi T. Characteristics of periodically domain-inverted LiNbO3 and LiTaO3 waveguides for second harmonic generation. <italic>Journal of Applied Physics</italic>. 1991; 70(4): 1947–1951. <ext-link xlink:type="simple" ext-link-type="doi" xlink:href="10.1063/1.349477">https://doi.org/10.1063/1.349477</ext-link></mixed-citation>
      </ref>
      <ref id="B15">
        <label>15</label>
        <mixed-citation xlink:type="simple">Ohlendorf G., Richter D., Sauerwald J., Fritze H. High-temperature electrical conductivity and electro-mechanical properties of stoichiometric lithium niobate. <italic>Diffusion Fundamentals</italic>. 2008; 8: 6.1–6.7. URL: <ext-link xlink:type="simple" ext-link-type="uri" xlink:href="https://nbn-resolving.org/urn:nbn:de:bsz:15-qucosa-192902">https://nbn-resolving.org/urn:nbn:de:bsz:15-qucosa-192902</ext-link></mixed-citation>
      </ref>
      <ref id="B16">
        <label>16</label>
        <mixed-citation xlink:type="simple">Zhukov R.N., Kiselev D.A., Ilina T.S., Temirov A.A., Kubasov I.V., Bykov A.S., Savchenko A.G. Effect of a Platinum Sublayer on the Microstructure and Spontaneous Polarization of Thin Lithium Niobate Films Deposited on a Silicon Substrate. <italic>Bulletin of the Russian Academy of Sciences: Physics</italic>. 2018; 82(9): 1232–1235. <ext-link xlink:type="simple" ext-link-type="doi" xlink:href="10.3103/s1062873818090265">https://doi.org/10.3103/s1062873818090265</ext-link></mixed-citation>
      </ref>
    </ref-list>
  </back>
</article>